Metal binder jetting and 'print-and-sinter' routes
📍 Where we are: Part II · Metal & Ceramic Processes — Chapter 7 of 15. Chapters 5 and 6 melted metal directly. Here the metal is shaped cold and fused later in a furnace, the same trick used by powder metallurgy for decades.
Think of a sandcastle made with a little glue mixed in. You can build it quickly and gently, because nothing is hot. It holds its shape, but it is fragile, and it is mostly air and glue. Now bake it until the glue burns off and the sand grains fuse together: the castle gets smaller and much stronger. Print-and-sinter metal works like that. The printer makes the fragile castle; the furnace makes it metal, and you have to plan for the shrinking.
What this chapter covers
Two printing methods feed the same furnace workflow. Metal binder jetting (see material and binder jetting for the printing step) deposits a liquid binder onto a bed of metal powder. Bound-metal extrusion, also called metal FFF or bound metal deposition (BMD), extrudes a rod or filament made of metal powder in a plastic binder, in the style of material extrusion. Both give a green part, which is then debound and sintered. We cover shrinkage, achievable density, geometry limits, and where the economics make sense, and we keep an eye on our lightweight bracket.
The workflow
- Print. Binder jetting prints with no heat and no supports in the powder, because the surrounding loose powder holds the part. Metal FFF prints at modest temperatures like any plastic extruder.
- Debind. The binder is removed, by solvent, by heat, or both. Solvent debinding followed by thermal debinding is a common sequence for metal FFF parts [1], and thermal debinding in the sintering furnace is also used [1]. What remains is a fragile brown part: metal particles barely touching.
- Sinter. In a furnace just below the melting point, the particles bond by diffusion and the pores shrink. The part densifies and shrinks as one object.
A green part is printed, the binder is removed, and sintering shrinks the part to a dense final size, so the model is scaled up beforehand.
Original diagram by the authors, created with AI assistance.
Shrinkage and compensation
A green binder jet part is typically only 40-60% of full (theoretical) density, because it is powder plus binder with lots of space between grains [2]. Sintering closes that space, so the part must shrink. For metal FFF, the review literature plots shrinkage against solid loading [3]. Binder jet parts also shrink substantially, and the exact figure depends on powder and settings [4].
Software compensates by printing the model larger than the final size. That works well when shrinkage is uniform, but it is not always uniform. In binder jetting, gaps between printed layers can cause anisotropic densification, and simulation that assumes isotropic shrinkage is least accurate in overhang areas [5]. Two further points:
- Binder jet work reports larger shrinkage in the build direction than in the plane [4]. Results differ between materials and machines, so measure your own.
- Gravity and friction against the furnace tray can distort large flat or thin parts, and long unsupported spans can sag; sintering simulation is used to predict this distortion [5]. Sintering may therefore need ceramic supports, called setters.
So the designer's job is to avoid long overhangs and large thin plates, keep thickness reasonably uniform, and allow for powder or binder escape.
Density and properties
Sintered parts can reach high density, but not always the fully dense state of a melted part. A review compiles sintered density against sintering temperature for 316L, 17-4PH and Ti-6Al-4V [3]. Residual porosity can remain after sintering, and post-sintering treatments such as hot isostatic pressing (HIP) are used when more density is needed; they add cost and can affect dimensions. Binder jet reviews discuss densification and post-heat-treatment in detail [4]. For fatigue-critical parts, remaining pores matter more than average density suggests. Check data for the exact material and furnace cycle, not a headline figure.
Where it fits economically
Print-and-sinter borrows its materials and furnaces from metal injection moulding (MIM), which makes small metal parts by injecting a powder-binder mix into a mould. MIM has expensive tooling but very cheap parts at high volume; print-and-sinter has no tooling, so it is generally argued to win at low and medium volume and for shapes a mould cannot make (the crossover depends on the part and on quotes, so we give no figure). The routes share feedstock concepts, debinding and sintering [3], and binder jetting is noted for high production rates [6]. Many parts can also share one furnace load, and nothing needs support structures during printing. The limits are:
- Furnace time and capacity. Debinding and sintering are long thermal cycles, so the furnace can become the bottleneck (an inference from the workflow, not a measured figure).
- Size and thickness. Binder must escape through the whole section, so thick sections are harder; check the supplier's limits.
- Accuracy and finish. Dimensional accuracy depends on predicting shrinkage [4], and good surface finish takes extra finishing steps.
These comparisons are qualitative; real cost depends on quotes.
The bracket test
Our lightweight bracket is small and made in a few hundred pieces a year. Binder jetting could print many at once in a stainless steel, sinter them together, and machine only the mounting faces; no tooling is needed. If it must be a thin, wide plate with long unsupported ribs, sintering distortion becomes the problem and PBF-LB may be safer. If a few thousand a year are needed and the shape is moulding-friendly, MIM might be cheaper. (All of this is qualitative; real cost depends on quotes.)
Why it matters
Print-and-sinter reaches metal AM without lasers, inert-gas handling or build supports, and makes it feasible for larger series. But it moves the difficulty to the furnace: dimensional control now depends on predicting shrinkage.
In the real world
Commercial metal FFF systems follow the print, debind and sinter workflow described in the reviews [1][3]. Reviews list the key control variables as powder, binder saturation, layer thickness and sintering temperature and time [4].
Key terms
- Green part — the printed, binder-held part before debinding and sintering.
- Brown part — a part after binder removal but before sintering, held together only weakly.
- Debinding — removal of the binder by solvent, heat or both.
- Sintering — heating just below the melting point so particles fuse and pores close.
- Shrinkage compensation — scaling the model up so the sintered part reaches the intended size.
- Bound metal deposition (BMD) / metal FFF — extrusion of metal powder bound in plastic, then debound and sintered.
- Setter — a ceramic support that holds a part during sintering to limit sagging.
- MIM — metal injection moulding, a high-volume sinter-based route using tooling.
- HIP — hot isostatic pressing, heat and gas pressure used to close remaining pores.
Where this leads
Sintering is also the central step for technical ceramics. Next: ceramics, composites and other material families.