Polymer powder bed fusion (SLS, MJF)

📍 Where we are: Part I · Polymer Processes — Chapter 3 of 15. Extrusion and vat processes need supports for overhangs; here the surrounding powder does that job, which changes how parts are packed and designed.

The simple version

Picture a tray of fine sugar. Run a hot wire over a pattern on the surface and the sugar along the line melts and sets into a solid line, while the sugar around it stays loose. Spread a fresh sugar layer on top and do it again. When you finish, you dig your sculpture out of a block of loose sugar. The loose sugar held everything up while you built, so you never needed scaffolding.

What this chapter covers​

We explain how polymer powder particles fuse, why polyamide 12 (PA12) is the workhorse, how the two main processes differ (laser sintering versus Multi Jet Fusion), how the powder is reused, and what properties and design freedoms result. In ISO/ASTM 52900 terms this is powder bed fusion: thermal energy selectively fuses regions of a powder bed [1]. SLS (selective laser sintering) and MJF (Multi Jet Fusion, a Hewlett-Packard process) are the common names.

From loose powder to a solid layer​

A machine heats the whole powder bed to just below the powder's melting point. Then energy raises the selected region over the melting point; particles soften, touch, and merge to close pores. The merging of two particles is driven by surface tension and resisted by viscosity: the sharper the heat pulse and the lower the melt viscosity, the more complete the fusion. Although the process is called sintering, a semi-crystalline polymer actually melts and then recrystallises on cooling, which is why bed temperature and cooling rate matter so much. A classic classification of laser sintering and melting by binding mechanism distinguishes solid-state sintering, chemically induced binding, liquid-phase sintering (partial melting) and full melting, and finds that most commercial processes fall into the last two [2].

Each cycle repeats: lower the build platform by one layer, spread new powder with a recoater (a roller or blade), heat, fuse. The unfused powder surrounds the part as a supporting cake. After the build, the whole cake cools slowly before being unpacked; the cooling time depends on the machine and the job, so follow the supplier's guidance.

Two ways to deliver energy​

AspectSLS (laser sintering)MJF (Multi Jet Fusion)
Energy deliveryA laser scans a point across the layerA printhead deposits a fusing agent where fusion is wanted and a detailing agent at the edges; an infrared lamp sweeps over the whole bed
Why it fusesThe powder absorbs laser lightThe fusing agent absorbs infrared, and the heat sinters the powder beneath it
EdgesSet by the laser spot and scan pathThe detailing agent inhibits fusion at the outline for sharper edges
Time per layerGrows with the area scannedLargely independent of how much of the layer is filled

In MJF, the fusing agent absorbs infrared radiation and the resulting heat sinters the powder, while the detailing agent inhibits fusion and so gives control of the part outline; the infrared source exposes the layer as a planar sweep rather than point by point [3].

Materials: why PA12​

Polyamide 12 (PA12, "nylon 12") dominates because it has a wide gap between melting and recrystallisation temperature, which lets the bed sit warm without caking and gives a stable process window; reviews single out its "outstanding position" among SLS polymer powders [4]. Polyamide 11 (PA11) is the other common polyamide; filled grades (glass, carbon or mineral filled) and thermoplastic polyurethane (TPU) powders give stiffer or flexible parts. PEEK is also listed among SLS materials, though it needs specialised high-temperature machines [5].

Powder reuse and refresh​

Powder that is heated but not fused is not wasted, but it ages: chains grow, colour yellows, and powder flow changes. To keep properties steady, operators blend used powder with new powder. The ratio of new to used powder is the refresh ratio. Reviews identify keeping the properties of laser-sintering polymers consistent as a continuing difficulty [6] and list poor reusability of unsintered powder as a drawback of SLS [5], so refresh policy is an economic lever as well as a quality one. Each machine and powder supplier gives its own recommended ratio; follow it.

Parts and properties​

  • No supports. Because the cake supports the part, you can build overhangs and interlocking assemblies, and nest many parts in 3D inside one build volume, which is why the process suits small production runs. Unfused powder must be removed from internal channels, so every enclosed cavity needs an escape hole.
  • Properties. SLS is described in reviews as giving the best mechanical properties and the least anisotropy among the polymer AM processes compared, though porosity is unavoidable in powder bed parts; surfaces are rough and the unsintered powder reuses poorly [5]. A 2022 review likewise credits SLS with needing no support structures and giving properties resembling injection-moulded parts, while noting porosity and a limited choice of polymers [7].
  • SLS versus MJF. Published PA12 comparisons depend on powder, machine and parameters. One benchmark found MJF specimens slightly stronger than SLS ones, which it attributed to the area fusion mode and a carbon black additive in the MJF powder [3], but this need not hold for other powders or machines, so compare supplier data for your own material and orientation.
  • Surface. A slightly grainy surface; bead blasting, tumbling or dyeing are typical finishes (see the post-processing chapter).
  • Shrinkage. Parts shrink as they cool, so machine software scales the model; large flat parts can still warp.

A cross-section of two polymer powder bed fusion machines side by side: SLS with a laser and scanner mirror, and MJF with a printhead carriage depositing fusing and detailing agents plus an infrared lamp, each showing a powder bed with a build piston, recoater and a part nested inside loose powder. SLS scans a laser over the layer; MJF prints fusing and detailing agents and sweeps an infrared lamp over the layer; in both, loose powder supports the part. Original diagram by the authors, created with AI assistance.

Bracket check​

This is the process that suits the (illustrative) bracket as a small series: pack dozens in a single build, no supports, no raft to snap off. Choose PA12 for a tough, usable part, and orient the rib so the load is not across the weakest direction. Keep wall thickness uniform, and add escape holes if any hollowing is used. Expect a matte grey surface and plan for blasting; bolt-hole faces may still need reaming.

Why it matters​

Polymer powder bed fusion is the polymer AM process closest to production. It needs no supports, uses a tough engineering polymer, and can print assemblies in one go. Its weak spot is the powder: the economics depend on how much can be reused without losing quality.

In the real world​

Service bureaus run fleets of SLS and MJF machines for functional prototypes and end-use parts such as housings, ducts and clips, with PA12 the most prominent powder [4]. The key practical questions are the refresh policy, cooling time and how parts are nested for density and thermal uniformity.

Key terms​

  • Powder bed fusion — AM process category where thermal energy selectively fuses regions of a powder bed.
  • SLS — selective laser sintering; a laser fuses the polymer powder.
  • MJF — Multi Jet Fusion; agents plus an infrared lamp fuse the powder.
  • Fusing agent — ink that absorbs infrared energy so the powder beneath it melts.
  • Detailing agent — ink that inhibits fusion at the edges to sharpen the outline.
  • PA12 — polyamide 12, the main polymer powder for SLS and MJF.
  • Powder cake — the block of loose powder that surrounds and supports the parts during the build.
  • Refresh ratio — the proportion of new powder blended with used powder.
  • Nesting — packing many parts in three dimensions inside one build.
  • Recoater — the roller or blade that spreads a new powder layer.

Where this leads​

Next: Material jetting and binder jetting, where inkjet-style printheads place drops of resin or binder.