Vat photopolymerization (SLA, DLP, LCD)
📍 Where we are: Part I · Polymer Processes — Chapter 2 of 15. Material extrusion used heat to fuse plastic; here the plastic starts as a liquid and a pattern of light solidifies it.
Imagine a dentist's blue light: a pasty filling is soft until the light shines on it, then it turns hard in seconds. Now imagine a vat full of that liquid, and a projector that shines one slice of your part into it. Only the lit region hardens, and it sticks to the part above. Lift the part a hair, shine the next slice, and repeat. The part grows out of the liquid, upside down, as if pulled from a pool.
What this chapter covers
We look at the chemistry that makes liquid resin solidify, the simple equation that predicts how deep a flash of light cures, the three ways of delivering light (laser, projector, LCD mask), the continuous variant called CLIP, the resin families, and why printed parts need a second cure. Vat photopolymerization is the ISO/ASTM 52900 category in which liquid photopolymer in a vat is selectively cured by light-activated polymerization [1]. SLA (stereolithography), DLP (digital light processing) and LCD (liquid-crystal display masking) are common names for its variants.
The chemistry: how liquid becomes solid
A resin is a mixture of monomers (small reactive molecules), oligomers (short chains with reactive ends), a photoinitiator, and additives such as pigment or light absorbers. Light of the right wavelength makes the photoinitiator split into reactive fragments that start a chain reaction, linking monomers into a cross-linked network: a solid thermoset.
Two chemistries dominate [2]:
- Free-radical polymerization of acrylates and methacrylates. Type I photoinitiators such as acyl phosphine oxides (TPO, BAPO) absorb towards 400 nm and bleach as they work, which helps light penetrate. It is fast, but dissolved oxygen inhibits it, especially in an open vat, and shrinkage is relatively high.
- Cationic polymerization of epoxides and vinyl ethers, started by onium salts such as aryl iodonium or triaryl sulfonium salts that release a strong acid. It is slower, shrinks less (epoxides are reported at 2 to 3 percent volumetric shrinkage) and can continue in the dark.
Many commercial resins are hybrids of both. Reviews of photopolymerization in 3D printing also cover red-shifted initiators, which move the working wavelength toward visible light [3].
The working curve: how deep does it cure?
Resin absorbs the light it receives, so the dose falls off with depth. The simplest model is the Jacobs working curve, adapted from the Beer-Lambert law of absorption:
Cd = Dp × ln(E / Ec)
where Cd is the cure depth, E is the exposure (energy per area), Dp is the penetration depth (where light intensity has dropped to 1/e), and Ec is the critical exposure, the dose at which the resin just reaches its gel point [4]. Plot cure depth against the logarithm of exposure and you get a straight line: the slope is Dp, and the intercept with zero depth gives Ec.
Use it as a guide, not a law. It assumes a monochromatic source and a response that does not depend on how fast the light arrives, and many modern printers and resins violate these assumptions. A 24-laboratory interlaboratory study found that fit parameters for the same resin differed by as much as 7 times for Dp and 70 times for Ec, showing that the measurement itself needs standardising [5].
Delivering the light
Reviews of the technology treat SLA, DLP and continuous DLP together and list the mechanical properties of the cured resins [6]. The main ways of exposing a layer compare as follows.
| Method | How the layer is exposed | Typical strengths | Typical limits |
|---|---|---|---|
| SLA (laser) | A UV laser spot is steered by mirrors and traces the slice | Fine, smooth features; large-format machines | Time grows with the area to be traced |
| DLP | A projector flashes the whole slice at once | Layer time independent of area | Pixel size sets resolution; projected area is limited |
| LCD (masked) | A UV LED panel shines through an LCD that blocks light except in the slice | Low cost, many pixels | Mask and light uniformity limit accuracy; mask wear |
In bottom-up machines the part hangs from a build plate and each layer is cured against a transparent window at the bottom of the vat; the part must then be peeled off the window, which loads thin features. In top-down machines the part sinks into the vat and a blade recoats the surface. All of them need supports for overhangs and to hold the part on the plate.
Continuous printing: CLIP
Peeling slows the build. In continuous liquid interface production (CLIP) an oxygen-permeable window creates a thin "dead zone" of liquid in which polymerization is inhibited, so the part is never stuck to the window and can be drawn upward continuously. The original paper reported complex solid parts drawn out at rates of hundreds of millimetres per hour, with feature resolution below 100 µm [7]. Because CLIP relies on oxygen inhibition, resin chemistries that suppress it, such as thiol-ene systems, are unsuitable [2].
Resins and post-cure
Resin classes include standard acrylate resins, tougher or flexible formulations, high-temperature and engineering-like resins, castable and dental or biocompatible resins, and ceramic- or filler-loaded resins. Typical limits: parts can be brittle, are sensitive to UV light and heat as they age, and the resin and uncured liquid need careful handling.
After printing, the "green" part is washed with solvent to remove uncured resin, then post-cured with light and often heat. Post-cure completes the conversion and improves strength and stability; cationic systems can be post-cured with light or heat, whereas (meth)acrylate resins are generally post-cured with light [2]. Post-curing also reduces anisotropy [2]. Washing and curing are covered further in the post-processing chapter.
Light from below cures one layer of resin against the window while the part hangs from the build plate; the working curve links exposure to cure depth.
Original diagram by the authors, created with AI assistance.
Bracket check
Vat printing can make a fine, smooth, detailed bracket, ideal for a visual prototype or a fit check. Orient it so large flat faces are tilted rather than parallel to the window (reducing peel force), keep the rib thick enough to survive peeling, and add supports away from the bolt-hole faces. For a load-bearing plastic bracket, check the resin's ageing and temperature limits first: a standard photopolymer is usually not the best choice.
Why it matters
Vat photopolymerization delivers some of the finest feature detail and smoothest surfaces among polymer AM processes, which is why it dominates in dental models and aligner moulds, jewellery patterns and detailed prototypes. Its chemistry is also a platform: change the resin and you change the material.
In the real world
Dental laboratories print models and surgical guides with DLP or LCD machines, jewellers print castable patterns, and manufacturers use CLIP-type systems for production polymer parts. Typical resins are proprietary mixtures, so supplier data sheets and your own test coupons matter more than a general rule.
Key terms
- Vat photopolymerization — AM process category where liquid photopolymer in a vat is selectively cured by light-activated polymerization.
- Photoinitiator — a molecule that absorbs light and creates the reactive species that start polymerization.
- Monomer / oligomer — the small and short-chain building blocks of the resin.
- Cross-linking — joining polymer chains into a three-dimensional network, which makes the part solid.
- Cure depth (Cd) — how deep into the resin a given exposure solidifies it.
- Jacobs working curve — the relation
Cd = Dp ln(E/Ec)between cure depth and exposure. - Penetration depth (Dp) / critical exposure (Ec) — the two resin parameters of the working curve.
- Oxygen inhibition — dissolved oxygen stopping free-radical polymerization; exploited by CLIP.
- CLIP — continuous liquid interface production, using an oxygen-permeable window and a "dead zone".
- Post-cure — a second exposure to light and/or heat that completes polymerization.
Where this leads
Next: Polymer powder bed fusion (SLS, MJF), where the powder itself holds the part while it is made.