Your first print
📍 Where we are: Part 3 · Getting Hands-On — Chapter 9 of 11. Parts 1 and 2 were about ideas and decisions. Now we make something, using the most common and cheapest kind of printer: a desktop filament printer.
A desktop printer is a very careful hot-glue gun on rails. It melts a thin plastic string, squeezes it out of a tiny hole, and draws one flat outline after another, each on top of the last, until a solid object appears. Almost everything that goes wrong comes down to one of three things: the first line of plastic did not stick to the plate, the plastic was too hot or too cold, or not enough plastic came out. Learning to read those three signs is most of what "getting good at printing" means.
What this chapter covers
We follow a first print of a small, simple object on a desktop machine that uses material extrusion, the process category in which a heated nozzle pushes material out and lays it down [1]. The popular name for it is FDM (fused deposition modeling) or FFF (fused filament fabrication). We cover choosing a machine, preparing the plate, the all-important first layer, the slicer settings that matter, and the three classic failures. Specific temperatures and settings depend on your printer and filament, so treat any numbers here as examples and rely on your printer maker's profiles.
How the machine works
The printer has a few key parts:
- Filament — the plastic "string", wound on a spool.
- Extruder — a motor and gears that grip the filament and push it forward.
- Hot end and nozzle — a heated block that melts the plastic, with a small metal tip (the nozzle, with an opening often around 0.4 mm wide) that the molten plastic leaves through.
- Build plate (or bed) — the surface the part is printed on, often heated.
- Motion system — motors and rails that move the nozzle and plate so the nozzle can draw anywhere in the build space.
Before printing, software called a slicer cuts the 3D model into layers and writes the nozzle's route as G-code, a simple text list of movement and temperature commands. Book 1's digital workflow chapter explains this chain; here we use it.
A filament printer in cross-section, and the three first-layer cases you will learn to recognise: nozzle too high (weak grip), correct (slightly squished), too low (blocked flow).
Original diagram by the authors, created with AI assistance.
Choosing a machine class
For a beginner, three broad choices matter more than brands:
- A ready-assembled, calibrated printer is the easiest way to learn. Printer makers' own documentation notes that factory-assembled printers are already tuned and that first-layer calibration is only needed for self-assembled kits or after changes such as a nozzle swap [2].
- A kit teaches you how the machine works, but takes longer and has more things to get wrong.
- Enclosed or open? An enclosed machine keeps warm air around the part, which helps with materials that warp (see below), and also contains fumes, a point we come back to in the safety chapter. An open machine is simpler and cheaper.
Start with PLA, a common beginner plastic that prints at a relatively low temperature and is generally more forgiving than higher-temperature materials such as ABS or ASA. One printer maker's knowledge base lists, as an example, 215 °C for the first layer and 210 °C for the others when printing its PLA on its own printers [3]. Always check your filament spool and your printer's profile instead.
Step by step
- Pick a simple model. A small calibration cube or a flat-bottomed object with no overhangs (parts that stick out over empty space) is ideal.
- Clean the plate. Fingerprint grease is a common cause of poor sticking. Wipe the plate as your printer's instructions say.
- Load the filament and let the printer heat the nozzle to the right temperature.
- Set the first-layer height. This is the single most important step, described next.
- Slice the model using the printer's recommended profile. Beginners rarely need to change anything except, perhaps, adding a brim (a thin flat skirt around the part's base that increases grip).
- Start the print and watch the first layer. Be present for the first few minutes.
- Let the part cool, then remove it. Many plates are flexible and release the part when bent.
The first layer
The first layer decides the whole print. The aim of first-layer calibration is to set the distance between the nozzle tip and the plate so that the extruded plastic sticks well and is slightly squished, as one manufacturer puts it [2]. There are three cases:
- Nozzle too high: the plastic comes out as round strands that barely touch the plate and can be dragged away.
- Nozzle just right: neighbouring lines melt together into a smooth flat sheet.
- Nozzle too low: the nozzle squeezes against the plate, and the filament cannot get out. Printer maker Prusa's guidance warns that a nozzle too close to the plate can obstruct the filament flow [4], and cautions against lowering the height setting too far to fix poor sticking, because it can damage the plate [5].
Different plate surfaces (smooth, textured) need different adjustments, so recalibrate when you change plate [2].
Three common failures and what they mean
Warping
Warping is when the corners of a part lift off the plate. Plastic shrinks as it cools; if the bottom cools while the top is still hot, the part curls. It is mostly seen with higher-temperature materials such as ABS, ASA and PC blends, and is caused by the temperature difference between the molten plastic and the surrounding air. A thin layer of glue stick on the plate can improve adhesion [6]. Other usual remedies are a brim and, for ABS, an enclosure.
Stringing
Stringing is thin hair-like threads between separate parts of the model, left because plastic oozes from the nozzle while it travels. It is caused by very high printing temperatures and/or wrong retraction settings (retraction means the extruder pulls the filament back slightly before a travel move) [7]. Remedies: lower the temperature a little, use the maker's retraction profile. Also try a different spool: the maker's troubleshooting page notes that filament that has picked up moisture can cause a lot of stringing [7].
Under-extrusion
Under-extrusion means not enough plastic comes out: gaps in layers, thin walls, and fragile parts. The first thing to check is the first-layer calibration (a nozzle too close can obstruct flow), then whether the nozzle is partly clogged, then whether the filament feeds smoothly from the spool [4].
| Symptom | Most likely cause | First thing to try |
|---|---|---|
| Part lifts at corners | Fast cooling, weak grip | Clean plate, add brim, glue stick |
| Hair-like threads | Too hot, retraction | Maker's profile, slightly lower temperature, dry filament |
| Gaps, thin or weak walls | Not enough plastic out | Re-do first-layer calibration, check for clog |
| First layer not sticking | Nozzle too high, dirty plate | Re-calibrate height, clean plate |
No printer yet? Start virtual
You can practise the digital half of printing without any hardware: slicing a model, reading the G-code, and watching a simulated printer run it. Book 3's labs walk through this with a virtual printer, in the virtual printer lab. It will not teach you the feel of a first layer, but it makes the later steps far less mysterious.
A word on safety
A hot nozzle burns, moving parts pinch, and heated plastic gives off tiny particles and vapours. Print in a ventilated space and never leave a printer running unattended in a place where a fire would go unnoticed. The next chapter covers this properly.
Why it matters
A first successful print teaches more than any chapter can. It also shows you that the clean, digital picture from earlier chapters meets the physical world: heat, sticking, shrinking and flow.
In the real world
Experienced users treat each failure as information. Print a small test, change one setting at a time, and write down what you changed. Printer makers' knowledge bases (for example the troubleshooting articles cited here) are valuable because they are written for the specific machine.
Key terms
- Material extrusion — the process category where a heated nozzle pushes material out and deposits it layer by layer.
- FDM / FFF — fused deposition modeling / fused filament fabrication: the common names for filament-based material extrusion.
- Filament — the thin plastic string, usually on a spool, that feeds an FDM printer.
- Nozzle — the small heated tip through which melted plastic is pushed out.
- Build plate — the surface on which the part is printed, often heated.
- Slicer — software that cuts a 3D model into layers and plans the nozzle path.
- G-code — the text-based list of movement and temperature commands a printer follows.
- First layer — the bottom layer of the part; its grip decides whether the print succeeds.
- Brim — a thin, flat extension around a part's base that increases grip on the plate.
- Retraction — pulling the filament back slightly before the nozzle travels, to reduce oozing.
- Warping — corners of a printed part lifting off the plate as the plastic cools and shrinks.
Where this leads